THQ80-1 is a low-alloy solid GMAW wire listed for 800 MPa class steel structures. Its value in selection comes from reading the published strength, impact, gas, and operating data together—and knowing which questions still need a test report or procedure record.
01What THQ80-1 is intended to do
Bridge Brand lists THQ80-1 as an AWS A5.28 ER110S-G low-alloy solid wire for gas metal arc welding of 800 MPa class high-strength steel structures. Its product page identifies construction machinery, vehicle manufacture, and structural steelwork among the intended applications. These application descriptions establish a starting point for selection, not automatic acceptance for every steel used in those sectors. [1]
The published setup uses M21 shielding gas and direct current electrode positive (DCEP). The mechanical-property description specifically identifies 80% argon and 20% carbon dioxide. Keep that gas composition attached to the reported results when comparing the wire with an existing welding procedure.
AWS's public description of A5.28/A5.28M:2026 confirms that the specification addresses low-alloy steel electrodes and rods for gas-shielded welding. It does not independently certify this particular product. The shop lists A5.28 without an edition; confirm the required edition and supporting documents for the actual order. [2]
02Read the requirement and typical-result columns separately
The following values reproduce the current Bridge Brand product data. The requirement column is the manufacturer's published product requirement; the typical column records its reported example result. These are not new tests performed for this article.
| Property | Published requirement | Reported typical result |
|---|---|---|
| Rm (MPa) | 770–940 | 823 |
| ReL / Rp₀.₂ (MPa) | ≥690 | 751 |
| A (%) | ≥17 | 19 |
| KV₂ (J) at −40 °C | ≥69 | 84 |
The 823 MPa typical tensile result sits within the published 770–940 MPa range. It should not replace that range in an order or be presented as a minimum that every production weld will achieve. Likewise, the listed 751 MPa typical yield result is different from the published minimum of 690 MPa. Review tensile and yield requirements separately rather than reducing both to an “800 MPa wire” label.
The product page associates these results with 80% argon and 20% carbon dioxide shielding, but does not provide a complete test report identifying the lot, weld preparation, heat input, thermal history, and specimen details. Obtain that evidence where the contract requires it. Published product values support initial screening; they do not replace the relevant material certificate or procedure qualification record. [1]
03Keep the −40°C impact value tied to its test
The published impact entry is KV₂ at −40°C: a minimum of 69 J and a typical result of 84 J. Keep the temperature, energy, and distinction between requirement and typical result together. Reporting “84 J toughness” without those boundaries loses information needed for comparison.
That result describes the reported weld-metal test, not a minimum service temperature for an entire structure. It also does not establish the toughness of the parent steel or heat-affected zone (HAZ). Those regions need the evidence required by the project. Do not translate a Charpy entry directly into a fracture-toughness value or a claim of suitability for any low-temperature duty.
A useful technical enquiry asks for the test condition, specimen size, sampling location, applicable acceptance rule, and traceable report. If those differ between two suppliers' data, resolve the difference before treating their impact numbers as directly comparable.
04Use the stated gas and diameter data as a starting point
The store lists reference currents by wire diameter: 0.8 mm at 50–180 A, 1.0 mm at 70–230 A, 1.2 mm at 80–350 A, and 1.6 mm at 120–500 A. These are manufacturer reference ranges, not a complete welding parameter schedule. They do not show that every current in a range suits every joint, position, or transfer mode. [1]
For a production trial, connect the selected diameter and current with the WPS requirements for voltage, wire feed, travel speed, contact-tip-to-work distance, gas delivery, joint detail, and thermal control. The product's listed positions are PA, PB, PC, PD, PE, and PF; the list should not be expanded to include an unlisted progression.
If the available gas differs from the stated 80/20 mixture, do not carry over the mechanical-property figures as an unchanged guarantee. Review the change with the supplier and welding coordinator and establish the evidence required for the revised procedure. The same discipline applies to a change in heat-treatment condition.
05Select for the actual joint, not the highest number
THQ80-1 should be considered when its documented properties and usability meet the joint requirements. “Higher strength” alone is not an instruction to substitute it for another filler. TWI describes matching, undermatching, and overmatching as relationships between weld and parent material; the relevant relationship must be defined for the application. [3]
TWI's May 2003 paper on softened HAZs examined specific quenched-and-tempered steels using bend specimens and mini-wide plate tests. It found that strength mismatch influenced the measured HAZ fracture toughness and stressed that assessment specimens must represent the practical mismatch condition. Those results explain why a stronger deposit cannot by itself settle a joint assessment; they are not a test of THQ80-1 or a prediction of its performance in an unspecified steel. [4]
Keep the product review focused: confirm the steel grade and delivery condition, required weld-metal strength and impact performance, shielding gas, welding position, and qualification coverage. Refer to the existing high-strength-steel guide for the wider hydrogen and thermal-control plan rather than inventing a universal preheat or heat-input limit for this wire.
06Make the product enquiry specific enough to verify
- Identify THQ80-1, the required ER110S-G classification documentation, wire diameter, and order traceability.
- State the actual parent steel, joint detail, position, service requirements, and applicable WPS.
- Request the required lot or conformity documents and the test basis for strength and impact results.
- Resolve any required approval scope using a current certificate covering the product and supply; a catalogue reference alone does not establish project acceptance.
- Verify the selected setup and required weld/HAZ properties through the applicable qualification and inspection plan.
This enquiry turns the published product information into a checkable selection. It avoids treating a typical result, an application label, or a spool photograph as proof of the finished joint's performance.
Connect the Product Sheet to the Welding Requirement
Use THQ80-1's published data to ask precise questions about the intended application. Preserve the test conditions and document the selected procedure so that purchasing, welding, and inspection work from the same evidence.
Related BBKP Resources
Technical References
- [1] Bridge Brand — THQ80-1 (ER110S-G), current product description and specification tables
- [2] AWS — A5.28/A5.28M:2026, public scope description
- [3] TWI — What Is Weld Metal?
- [4] TWI — The Significance of Softened HAZs in High Strength Structural Steels (May 2003)
Product data checked on November 17, 2026. Numerical product values above come from Bridge Brand's current store records, not an independently witnessed test or a newly commissioned experiment. The cited TWI study concerns its stated steels and conditions. Confirm current supply documents and project requirements before production use.